产品描述

NORYL PPO EN110物性表

NORYL EN110 is an extrusion material with a Vicat B/120 of 115oC according ISO 306. NORYL EN110 is a standard extrusion grade for applications where medium temperature resistance is required.

TYPICAL PROPERTIES (1)
MECHAN ICAL机械性能
Value Unit Standard
Tensile Stress, yield 50 mm/min / 抗张程度,屈服, 50 mm/min
45
MPa
ISO 527
Tensile Stress, break, 50 mm/min / 抗张程度,断裂,50mm/min
40
MPa
ISO 527
Tensile Strain, yield, 50 mm/min / 拉伸伸长,屈服,,50mm/min
3
%
ISO 527
Tensile Strain, break, 50 mm/min / 拉伸伸长,断裂,50mm/min
30
%
ISO 527
Tensile Modulus, 1 mm/min / 拉伸模量,1 mm/min
2200
MPa
ISO 527
Flexural Stress, yield, 2 mm/min / 弯曲强度,屈服,2 mm/min
60
MPa
ISO 178
Flexural Modulus, 2 mm/min / 弯曲模量,2 mm/min
2000
MPa
ISO 178
Hardness, H358/30 / 球压硬度,H358/30
87
MPa
ISO 2039-1
IMPACT
Value Unit Standard
Izod IMPACT, notched 80*10*4 +23°C / 悬壁梁缺口冲击强度,80*10*4 +23°C
11
kJ/m2
ISO 180/1A
Izod IMPACT, notched 80*10*4 -30°C / 悬壁梁缺口冲击强度,80*10*4 -30°C
5
kJ/m2
ISO 180/1A
Charpy 23°C, V-notch Edgew 80*10*4 sp=62mm / 简支梁缺口冲击强度,23°C,C80*10*4 sp=62mm
11
kJ/m2
ISO 179/1eA
Charpy -30°C, V-notch Edgew 80*10*4 sp=62mm / 简支梁缺口冲击强度,-30°C,C80*10*4 sp=62mm
5
kJ/m2
ISO 179/1eA
THERMAL
Value Unit Standard
Thermal Conductivity / 导热系数
0.23
W/m-°C
ISO 8302
Ball Pressure Test, 75°C +/- 2°C
PASSES
IEC 60695-10-2
Vicat Softening Temp, Rate A/50 / 维卡软化温度 A级/50
120
°C
ISO 306
Vicat Softening Temp, Rate B/50 / 维卡软化温度 B级/50
115
°C
ISO 306
Vicat Softening Temp, Rate B/120 / 维卡软化温度,B级/120
115
°C
ISO 306
HDT/Be, 0.45MPa Edgew 120*10*4 sp=100mm / 热变形温度,0.45 MPa, 未退火, 100 mm 跨距
100
°C
ISO 75/Be
HDT/Ae, 1.8 MPa Edgew 120*10*4 sp=100mm / 热变形温度,1.8 MPa, 未退火, 100 mm 跨距
95
°C
ISO 75/Ae
PHYSICAL
Value Unit Standard
Mold Shrinkage on Tensile Bar, flow (2) / 收缩率,流动
0.5 – 0.7
%
SABIC Method
Density/密度
1.05
g/cm3
ISO 1183
Water Absorption, (23°C/sat) / 吸水率, (23°C/sat)
0.15
%
ISO 62
Moisture Absorption (23°C / 50% RH) / 吸水率, 平衡,(23°C / 50% RH)
0.06
%
ISO 62
Melt Volume Rate, MVR at 280°C/3.8 kg
15
cm3/10 min
ISO 1133
ELECTRICAL
Value Unit Standard
Volume Resistivity/体积电阻率
1.E+15
Ohm-cm
IEC 60093
Surface Resistivity, ROA / 表面电阻率
>1.E+15
Ohm
IEC 60093
Dielectric Strength, in oil, 3.2 mm / 耐电强度,在油中,3.2mm
19
kV/mm
IEC 60243-1
Relative Permittivity, 50/60 Hz / 相对介电常数,50/60 Hz
2.6
IEC 60250
Relative Permittivity, 1 MHz / 相对介电常数,1 MHz
2.6
IEC 60250
Dissipation Factor, 50/60 Hz / 耗散因素,50/60 Hz
0.004
IEC 60250
Dissipation Factor, 1 MHz / 耗散因素,1 MHz
0.001
IEC 60250
FLAME CHARACTERISTICS
Value Unit Standard
UL Compliant, 94HB Flame Class Rating (3)(4)
1.65
mm
UL 94 by GE
Oxygen Index (LOI) / 极限氧指数
22
%
ISO 4589
Source GMD, last updated:10/31/1995
Processing
Parameter
Profile Extrusion
Value Unit
Drying Temperature / 干燥温度
80 – 100
°C
Drying Time / 干燥时间
2 – 3
hrs
Melt Temperature / 熔体温度
260 – 300
°C
Calibrator Temperature
60 – 80
°C
Source GMD, last updated:10/31/1995